Pwosedi soude nan A606 Plak Steel Weathering

1. Materyèl Apèsi sou lekòl la (A606 Steel)

Lèt: Weathering asye (menm jan ak ASTM A588, Corten)

Kle alyaj: Cu, Cr, Ni, P (amelyore rezistans korozyon)

Sede fòs: 345 MPa (50 ksi) min

Karakteristik remakab: Fòme yon kouch rouye pwoteksyon ("patin") sou tan


2. Preparasyon pre-soude

(1) Netwayaj sifas yo

Deplaseechèl moulen, rouye, lwil, oswa pentiSèvi ak fanm k'ap pile, sandblasting, oswa netwayaj chimik.

Asirebor jwenti yo pwòp(pa gen okenn kontaminan).

(2) Joint Design & Fit-up

Rèlte: ItilizeV-Groove, J-Groove, oswa U-Groove for thick plates (>6mm).

Gap kontwòl: Kenbe1.5-3mm rasin rasinpou plen pénétration.

Chofe (si sa nesesè):

Chofe temp: 50-150 degre (depends on thickness, typically needed for >20mm plak).

Entèrpass temp: Mwens pase oswa egal a200 degre(Pou evite twòp chalè opinyon).


3. Metòd soude & consommables

(1) Pwosesis Rekòmande

Metòd Pi bon pou Nòt
SMAW (baton) Soude jaden, reparasyon Sèvi ak branch ki ba-idwojèn
GMAW (MIG) Pwodiksyon segondè-vitès Mande pou pwoteksyon gaz (AR+CO₂)
Fcaw (flux-cored) Plak lou, soude deyò Pwòp tèt ou-pwoteksyon oswa gaz-pwoteksyon
Gtaw (tig) Presizyon, plak mens High-bon jan kalite fini

(2) seleksyon metal filler

Klasifikasyon AWS:

Smaw: E7018-W(ba-idwojèn, klas dezagregasyon)

Gmaw/fcaw: ER70s-6(pou asye modere) oswaEwni-1(pou pi bon matche ak korozyon)

Gtew: ER70s-2(Cleaner Weld)

Biyè: Si matche pwopriyete dezagregasyon se kritik, itilizeCorten-espesifik file (e.g., AWS A5.28 ER80S-NI1).


4. Paramèt soude

(1) Anviwònman tipik

Trete Kouran (a) Vòltaj (V) Vitès vwayaj Gaz (si yo itilize)
Smaw 90-140 (DC+) 22–28 Modere N/A
Almaw 150–250 22–30 Rapid 75% ar + 25% co₂
Fcaw 180–300 24–32 Mwayen Co₂ oswa pwòp tèt ou-pwoteksyon

(2) Kontwòl D 'chalè

Max chalè opinyon: Mwens pase oswa egal a 2.5 kJ/mm(Pou evite haz fragliseness).

Teknik:

Isajpèl stringer(Evite twòp resi).

Multi-Pass soudepou plak epè.


5. Tretman pòs-soude

(1) to refwadisman

PèmètRefwadisman natirèl(Evite asouvisman).

(2) Tretman chalè pòs-weld (PWHT, si sa nesesè)

Estrès soulaje: 550-650 degre(pou aplikasyon kritik).

(3) Sifas fini

Moulen: Smooth Weld Couture matche ak baz metal.

Fòmasyon patin:

Weathering asye praldevlope rouye sou tan(pa bezwen pou penti).

Si pentire obligatwa, itilizePremye-konpatib prime.


6. Enspeksyon & Kontwòl Kalite

Enspeksyon vizyèl (VT): Tcheke pou fant, porosite, koupe.

NDT (si sa nesesè):

Dye penetran (PT)pou domaj sifas yo.

Ultrason (UT)ouRadyografi X-ray (RT)pou defo entèn yo.

Tès dite: Asire dite haz mwens pase oswa egal a350 hv.